Heerarka deegaanka EU RoHS 2.0 waxay codsanayaan in maadada rasaasta (Pb) ay ka yar tahay 1000ppm. Iyada oo ku saleysan shuruudahan, KINKOU waxay soo saartay C17300-lead hooseeya iyo wax qabadkeeda goyntu waxay la mid tahay C17300 .Waxqabadka goynta ee C17200 sidoo kale waa wanaagsan yahay.
1. Waxyaalaha kiimikaad ee rasaasta hoose ee C17300
Qaabka | Be | Ni+Co | Ni+Co+Fe | Pb | Cu |
C17300 | 1.8-2.0 | ≥0.20 | ≤0.6 | 0.1 | Haraaga |
2. Qalabka Jirka iyo Makaanikada eehogaanka hooseC17300
Gobolka | Daawaynta kulaylka (℃) | Dhexroorka (mm) | Xoogga Jilitaanka (MPa) | Xoogga Wax-soo-saarka (MPa) | Dheeraynta 4xD (%) | Adag | Waxqabadka Korontada (IACS,%) | |
HV0.5 | HRB ama HRC | |||||||
TB00 | 775 ℃ ~ 800 ℃ | Dhammaan | 410-590 | >140 | >20 | 159-162 | B45-B85 | 15-19 |
TD04 | 775 ℃ ~ 800 ℃ Xalka+ adkeynta Habka Qabow | 8-20 | 620-860 | >520 | :8 | 175-257 | B88-B102 | 15-19 |
0.6-8 | 620-900 | >520 | :8 | 175-260 | B88-B103 | |||
TH04 | 315 ℃ x1 ~ 2 saac | 8-20 | 1140-1380 | >930 | >20 | 345-406 | C27-C44 | 23-28 |
0.6-8 | 1210-1450 | >1000 | >4 | 354-415 | C38-C45 |